Dear Mr. Parveen K. Nakwal
If construction code is ASME refer Sec. VIII Div. 1 UCS 56
For Heating
Above 800°F (425°C), the rate of heating shall
be not more than 400°F/hr (222°C/ h) divided by the maximum
metal thickness of the shell or head plate in inches,
but in no case more than 400°F/hr (222°C/h).
For cooling
Above 800°F (425°C), cooling shall be done in
a closed furnace or cooling chamber at a rate3 not greater
than 500°F/hr (280°C/h) divided by the maximum metal
thickness of the shell or head plate in inches, but in no
case more than 500°F/hr (280°C/h).
Note : The rates of heating and cooling need not be less than 100°F/hr
(56°C/h). However, in all cases consideration of closed chambers and
complex structures may indicate reduced rates of heating and cooling to
avoid structural damage due to excessive thermal gradients.
With Best Regards
Nagarajan B
Parveen Kumar Nakwal ---13/06/2012 16:49:25---Dear Experts. What is the tolerance limit of Rate of heating and cooling in PWHT process
From: Parveen Kumar Nakwal <pknakwal@gmail.com>
To: materials-welding@googlegroups.com
Date: 13/06/2012 16:49
Subject: [MW:14530] Tolerance of Rate of heating & cooling
Sent by: materials-welding@googlegroups.com
Dear Experts.
What is the tolerance limit of Rate of heating and cooling in PWHT process ? Please mention Section & Clause no.
Waiting for reply.
Parveen K. Nakwal
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment